Material / Aluminum ADC12 (AlSi10Cu2Fe)

ADC12 aluminum die casting: the Japanese standard read against the drawing

ADC12 arrives on drawings from Japanese and Asian supply chains. It fills slightly better than A380, wears better, and gives up a little ductility to get there.

ADC12 Die Casting material review ADC12 Die Casting material review
9.6–12.0%
Silicon, higher than A380
≈ 310 MPa
Typical as-cast tensile strength
1–3%
Elongation, the ductility cost
580–620 °C
Melt temperature window
01 / Why this alloy

What ADC12 is chosen for

ADC12 is the JIS H 5302 designation most Asian drawings use. Its silicon runs higher than A380 at roughly 10–12%, which buys fluidity and wear resistance: thin walls fill further, and a sliding face survives longer. Copper sits around 1.5–3.5%, enough for strength without the full hot-shortness of a high-copper alloy.

The alloy is common in electronic chassis, motor end covers, transmission covers and general machinery housings, especially where the drawing already names ADC12 and the supply chain is Asian. It is also the usual fallback when a part is being transferred from a Japanese supplier and nobody wants to re-qualify an alloy.

Two costs come with it. Ductility is lower than A380 — 1–3% elongation is normal — so a design that relies on the part bending before it breaks is already in trouble. And the higher silicon makes machining more abrasive on the tool, which shows up in tool life rather than in the cycle time. The worked cost example shows which lines dominate the price of a 320 g cover, and why the alloy line is usually the smallest of them.

  • Electronic chassis and covers
  • Motor end shields and transmission covers
  • General machinery housings
  • Parts transferred from a Japanese or Asian supply chain
  • Components that see sliding wear rather than impact
02 / Composition

Typical composition and the tolerance that matters for each element

Ranges follow the JIS H 5302 ADC12 family. The heat certificate controls the lot; the spectrometer on the melt controls the shot.

ElementTypical range, wt%What it controls
Si9.6–12.0Fluidity and wear resistance. The top of the range is what makes thin-wall filling possible
Cu1.5–3.5Strength and hardness. Higher copper means more hot shortness
Mg≤ 0.30Strength through Mg2Si; also gas pickup if it drifts high
Fe≤ 1.30Die sticking versus brittle iron phases; the classic trade-off
Mn≤ 0.50Controls the shape of the iron phases
Zn≤ 1.00Tramp; tolerated but watched
Ni≤ 0.50Usually tramp; can improve elevated-temperature strength
Sn≤ 0.30Tramp; lowers strength
AlbalanceThe matrix
ADC12 and A380 are not interchangeable on paper even where they behave similarly in the die. If a customer drawing says ADC12 and the foundry proposes A380, the substitution is a documented deviation, not a purchasing decision.
03 / Properties

Mechanical and physical properties, as cast

Typical values for separately cast test bars; a real casting depends on wall thickness, gate position and porosity.

PropertyTypical valueHow the drawing uses it
Ultimate tensile strength≈ 310 MPaSection sizing, bolted joints
Yield strength, 0.2%≈ 160 MPaClamp load and thread engagement
Elongation1–3%Drops, impact and crash arguments
Hardness≈ 74–95 HBWear at sliding faces, machining feeds
Density2.70 g/cm³Part weight
Thermal conductivity≈ 92–96 W/m·KHeat spreading in covers and chassis
Melting range≈ 580–620 °CDie temperature and cycle
The elongation figure is the one buyers underestimate. A 1–3% alloy is fine for a housing in compression and poor for a bracket that has to absorb a hit; ask which one the drawing describes.
04 / Casting behavior

How ADC12 behaves inside the die

Fluidity and thin walls

The high silicon eutectic keeps ADC12 fluid down to 0.8–1.0 mm walls, which is why it turns up on electronic chassis and covers with fine ribs. Gate velocity still rules the fill: 30–60 m/s with a die at 180–250 °C.

Because the alloy is more forgiving on fill, the failure mode shifts. A badly gated ADC12 part does not show cold shuts; it shows porosity in the last-to-freeze section, which is only found by X-ray or by a leak test.

Shrinkage and ejection

Shrinkage is similar to A380 at roughly 0.5–0.7% linear. The higher silicon does make the casting slightly more brittle at ejection, so ejector pin marks on a thin wall can turn into cracks if the wall is under 1.2 mm and the pin is close to an edge.

Draft below 1° on an outside wall is the usual cause of drag marks; on deep pockets 0.5° can work, but only with a polished die and a release agent under control.

Porosity and pressure tightness

ADC12 is used for covers and housings that must keep dust, water or oil out. The mechanism is the same as any aluminum die casting: gas from turbulence, shrinkage at the hot spot. Vacuum assistance and overflow placement do most of the work.

For electronic chassis the requirement is usually IP rather than pressure. The gasket groove geometry and the flatness of its land matter more than the alloy; a 0.05 mm flatness spec across the groove is normal on a machined land.

05 / Machining and finishing

Machining, finishing and assembly notes

Machining

The silicon content makes ADC12 more abrasive than A380: expect shorter carbide life on long runs, and budget for PVD-coated inserts and a slightly lower surface speed, around 250–500 m/min.

Thin walls deflect under clamping, so the machining plan fixes the support and the order of operations before it fixes the feeds. Datum strategy is reviewed together with the casting datum, not after the first article.

Finishing

Powder coating, e-coat and chromate work normally. Anodizing is not a cosmetic option: the silicon and copper produce a dark, mottled film, so visible parts are coated instead.

Where the part is a heat spreader, coating thickness matters: a 60–80 µm powder coat adds thermal resistance, so masked contact pads or a thinner e-coat are specified instead.

Assembly

ADC12 takes machined threads and cast-in inserts, and it machines a clean thread form. As with any die casting, engagement below 1.5× diameter is where pull-out failures start.

Welding is not a production method. For a chassis that needs a seam, the design uses a gasket, a folded joint, or a mechanical fastener rather than a weld.

06 / Alternatives

Where ADC12 sits against the other alloys

The comparison is usually ADC12 against the alloy your customer's other supplier already runs.

AlloyTensile, typicalElongationPick it when
A380≈ 324 MPa≈ 3.5%North American drawing, more ductility, easier machining
A360≈ 317 MPa≈ 3.5%Corrosion resistance or anodizing is required
Zamak 3 (zinc)≈ 280 MPa10–15%Thin decorative walls and plating; much heavier
If a part is transferred from an Asian supplier, keeping ADC12 avoids a re-qualification cycle even where A380 would work. The saving from switching is usually smaller than the cost of a new first article.
07 / Inspection

What is checked on an ADC12 part

CharacteristicMethodFrequency
ChemistrySpectrometer on the meltEvery heat
DimensionsCMM at 0.001 mm, or gaugesFirst article, then per-lot sample
Porosity in sealing or structural zonesX-ray, plus sectioningFirst article and periodic
Flatness on gasket or PCB landsCMM or surface platePer lot on machined lands
Cosmetic defectsApproved sample under agreed lightEvery lot
Threads and insertsGo/no-go gauge, pull test100% gauge, sample pull
Covers and chassis usually fail on flatness before they fail on strength. The flatness check is written against a stated datum and measured after machining, because the as-cast surface is not the assembly surface.
08 / Typical parts

Three parts where ADC12 is the natural call

An electronic chassis with 1.0 mm walls, internal ribs and a machined PCB land is the standard case. ADC12 fills the ribs, the land is machined flat, and the coating covers the outside while the contact pads stay masked.

A motor end shield or transmission cover adds a bearing bore and a sealing groove. The alloy supplies the fill; the datum strategy supplies the bore position; the inspection plan supplies the flatness evidence.

A general machinery housing where the drawing already says ADC12 is the least risky case of all: no substitution, no re-qualification, and the process window is already known from the previous supplier.

Buyer questions

ADC12 questions that change the quotation

Substitution, ductility, machining and coating are the four answers you will be asked for first.

Close, not the same. ADC12 allows more silicon (up to 12%) and often less copper; A380 allows 2–4% copper with 7.5–9.5% silicon. Both fill and machine well. ADC12 is slightly more fluid and more wear resistant, A380 slightly more ductile and easier on the tool. A substitution should be written as a deviation.

Because the high silicon eutectic and the copper phases leave little room for plastic deformation before cracking. Values of 1–3% are normal. It does not stop the alloy being used for housings, but it does mean a drop or crash case has to be argued with geometry, not with material ductility.

Only as a technical, non-cosmetic finish. Silicon and copper make the film dark and uneven, so visible parts are powder coated, e-coated or chromate treated. Where anodizing is a drawing requirement, A360 is the alloy to quote.

Yes, on the machining side. Carbide life on long runs is shorter than with A380, and the mitigation is coated inserts plus a slightly lower surface speed. Die life itself is governed by steel grade and maintenance, not by the silicon in the alloy.

0.05–0.10 mm across a machined land is normal, measured after machining against a stated datum. As-cast surfaces hold 0.15–0.30 mm at best. If the drawing asks for 0.05 mm without machining, the requirement needs a conversation before the die is cut.

Related pages

Where this page connects.

Material, process, product and RFQ pages around the same decision.

Send the drawing. Get the engineering questions first.

Include the material, annual quantity, finishing requirement, target market and delivery date. The review can start from STEP, IGS, DWG, DXF, PDF or ZIP files.

Start an RFQ
Upload drawing