Product / Hydraulic Pump Body

Hydraulic Pump Body die casting and machining

A hydraulic pump body is a pressure vessel with machined bores. Porosity that would be cosmetic elsewhere is a leak here, so gating, wall section and testing are designed together.

Hydraulic Pump Body engineering pattern Hydraulic Pump Body engineering pattern
Material
A380 / ADC12
Tooling
Vacuum assist, 1–2 slides
Machining
Bores + ports
Test
100% pressure test
01 / What the part does

A pressure vessel with a bearing bore

A hydraulic pump body holds the pumping elements, carries the shaft bearing and contains oil at working pressure. Its critical features are the bore that locates the pumping elements, the port threads that connect to the circuit and the wall that separates pressure from atmosphere.

The pressure zone is the part that decides the process. Die casting is used for low- and medium-pressure bodies, commonly up to 20–30 bar; above that the body usually moves to gravity casting, forging or steel. Within the die-cast range, the wall between a pressure gallery and the outside must be dense, and the gate must not place a weld line on it.

Failures are leaks, not fractures: oil weeps through connected porosity, a port thread strips under torque, or the bore wears because the pumping elements were not concentric. All three are controlled by design, machining sequence and a pressure test strong enough to catch what inspection cannot see.

  • Bore diameter, roundness and concentricity between bores
  • Pressure-zone wall thickness and porosity class
  • Port thread depth, squareness and pull-out strength
  • Flatness of the valve or cover face
  • Cross-hole intersections and burr control

Where this part sits in the wider picture: the constraints that come with industrial machinery, the numbers behind the tolerances in the pressure decay testing and leak limits, and the pump and valve body family this geometry belongs to.

02 / Design rules

Pressure, ports and bores

The pressure zone sets the wall; the ports set the threads; the bores set the machining plan.

FeatureWorking rangeWhy it matters
Pressure-zone wall3.5–5.0 mmThe wall must resist working pressure and stay dense. Thinner walls fill well but connect porosity to the outside more easily.
Bore stock0.5–0.8 mm on the radiusEnough to clean up core shift without cutting into the porous center of a thick section.
Port bossesWall ≥ 1× thread diameter; thread depth ≥ 1.5× diameterAluminum threads strip before steel fittings do. The boss is what carries the load.
Draft1–2° on walls; 0.5° minimum in port coresPort cores are thin and deep; insufficient draft breaks them or leaves flash in the thread zone.
Valve-face flatness0.02–0.05 mm after machiningThe valve plate or cover seals on this face; flatness sets the gasket or O-ring compression.
Porosity in pressure zoneNo connected porosity; X-ray acceptance zone stated on the drawingA pore that reaches the surface is a leak, not a cosmetic defect.
Cross-holesDeburred and blended; no sharp intersectionA burr at a cross-hole breaks free and travels into the pump.
Machined bore tolerance±0.01 mm; concentricity 0.02–0.03 mmPumping-element clearance and wear both depend on it.
Working pressure determines whether HPDC is the right process at all. Bodies above roughly 30 bar usually move to a different casting process or material.
Process route for a die-cast hydraulic pump body: A380 or ADC12, vacuum with 1-2 slides, valve face machined to 0.02 mm, 100% pressure test on every body.
Pressure decides a pump body. Wall thickness of 3.5-5.0 mm, vacuum-assist during filling and a stated X-ray acceptance zone are what keep the pressure gallery dense; the valve face is machined to 0.02 mm and every body is pressure tested, not sampled.
03 / Tooling

Gating so the pressure zone stays dense

Gate and weld-line control

Gate into a thick section away from the pressure zone, and arrange the fill so the last point to fill is not on a sealing face. A weld line that crosses the pressure wall is a line of weak, possibly porous metal exactly where the body must hold oil.

Vacuum assist is normal on pump bodies. It reduces gas entrapment in the thick sections and improves the density of the surfaces that will be machined into bores.

Slides and port cores

Port cores and cross-hole slides are thin, deep features that see the most wear. They are designed with adequate draft, their own cooling and a replacement strategy, because a damaged port core stops the tool faster than any other failure.

Every slide leaves a witness line. On a port boss, that line is placed outside the thread zone or on a face that is machined afterwards.

Thermal balance

The thick pressure wall cools last. Cooling is concentrated there so the wall solidifies while the gate is still feeding it; otherwise a shrink void forms in the middle of the wall, invisible from outside and connected to the bore after machining.

04 / Machining and datums

Bores, ports and cross-holes in the right order

Datum and bore sequence

Machine the mounting face and the first bore in one setup, then the second bore from the first as a reference so concentricity is held by the machine. Port faces are machined after the bores, because the port position is referenced to the bore axis, not the other way round.

Threads and cross-holes

Port threads are cut after the pressure test where the test fixture needs a plain bore, or tested through a fixture that seals on the thread. Cross-holes are drilled after the main bores so the burr can be removed from the inside, and the deburr operation is specified rather than left to the operator.

Thread depth and squareness are checked with go/no-go gauges and a thread-depth check on every lot. A thread that is square but shallow leaks at the fitting washer.

Pressure test

Bodies are tested 100% at 1.5× working pressure for a defined hold time, or by pressure decay where the specification allows. The test pressure, medium, hold time and allowed leak rate are drawing requirements, and the fixture is part of the production cell.

05 / Finishing and protection

Protect the outside without sealing the ports

Coating and masking

Pump bodies are usually conversion coated or painted. Threads, sealing faces, bore surfaces and the pressure-test ports are masked. Paint in a thread changes the torque and paint on a sealing face becomes a leak path.

Cleaning and contamination control

After machining, the body is cleaned and the internal passages are checked for chips. A hydraulic body that ships with a chip in a gallery fails at your customer and takes the pump with it, so cleaning and passage inspection are stated in the inspection plan.

Assembly scope

Where the program includes it, the body can leave with the bearing, seals, plugs and the valve plate fitted and the assembly pressure-tested as a unit.

06 / Inspection

Inspection plan for a pump body

The pressure zone is verified by X-ray and by test; the bores and threads are measured.

CharacteristicMethodFrequency
Bore diameter, roundness, concentricityCMMFirst article and every lot
Pressure-zone porosityX-ray, destructive section on first articleFirst article and periodic
Pressure tightness1.5× working pressure hold, or pressure decay100%
Port threadsGo/no-go gauges, torque test on sample100% gauges, sample torque
Valve-face flatnessCMM or surface plateEvery lot
Cross-hole burrsBorescope or flush checkEvery lot
Cleaning and passage contaminationFlush and filter checkEvery lot
The pressure-test record is the release document for this part family. A dimensional report alone does not prove the body holds oil.
07 / Failure modes

Where pump bodies usually go wrong

Leaks and contamination dominate this part family.

RiskHow it happensWhat removes it
Oil weeps through the pressure wallShrink porosity in a thick section, connected after machiningCool the thick wall, feed it from the gate, X-ray the zone
Thread strips under torqueThin boss or shallow threadIncrease boss wall and thread depth, torque-test the sample
Burr enters the circuitCross-hole drilled after deburr, or deburr not specifiedDrill cross-holes before the final deburr, specify the method
Valve face leaksFlatness lost after coating or handlingMask the face, check flatness after finishing
Bore wears earlyConcentricity or roundness out of specificationMachine both bores from one datum, check roundness per lot
A pump body that passes dimensions and fails pressure is a process problem, not an inspection problem. Fix it in gating and cooling.
Buyer questions

Hydraulic pump body questions that change the quotation

Working pressure, port threads and test method decide whether HPDC is the right process.

Typically up to 20–30 bar for HPDC bodies. Above that, pressure tightness and fatigue usually point to gravity casting, forging or steel. The working pressure and test pressure belong on the drawing before the process is chosen.

100% at 1.5× working pressure for a defined hold time, or by pressure decay where the specification allows. The medium, pressure, hold time and allowed leak rate are drawing requirements.

Threads are machined, not cast. Depth and squareness are gauged 100%, and pull-out or torque strength is verified on a sample. The boss wall is what decides whether the thread survives.

Both are used for low- and medium-pressure bodies. Selection follows pressure tightness, machining behavior and the finishing route rather than a large mechanical difference.

Yes. Where the program includes it, the body can leave with the bearing, seals, plugs and valve plate fitted and the assembly pressure-tested as a unit.

Related pages

Continue through the project path.

Material, process, industry and RFQ pages around the same decision.

Send the drawing. Get the engineering questions first.

Include the material, annual quantity, finishing requirement, target market and delivery date. The review can start from STEP, IGS, DWG, DXF, PDF or ZIP files.

Start an RFQ
Upload drawing