Capability / Zamak die casting

Zamak die casting, from alloy choice to a plated part

Zamak die casting is zinc die casting with a named alloy: Zamak 3 where plating uniformity decides the reject rate, Zamak 5 where strength and thread wear matter. This page covers the alloy family, the wall and tolerance the process holds, the plating decision and the inspection that has to happen before plating.

Zamak 3 die cast handset housing Zamak 3 die cast handset housing
0.5 mm
Thin wall on small Zamak parts
±0.025 mm
As-cast under 25 mm
Zamak 3 / 5 / 2 / ZA-8
Grades quoted on this page
15–25 days
Tool build after drawing release
01 / Alloy family

Why Zamak is chosen, and what it gives up

Zamak is a small family of zinc alloys with aluminum at 3.9–4.3% and copper as the variable: trace in Zamak 3, around 1% in Zamak 5, 2.5–3.5% in Zamak 2. They all melt near 385–390 °C, roughly 200 °C below aluminum, so the die sees less thermal shock, the cycle is short, and 0.5–0.8 mm walls fill without the gate velocity an aluminum die needs. That is the whole commercial reason zinc holds the small precision part.

The trade is density and metal price. Zinc is 6.6–6.7 g/cm³ against 2.7 for aluminum, so the same geometry is about two and a half times heavier, and zinc ingot costs more per kilogram. On a part sold by weight, or carried by hand at size, aluminum wins on material. On a small, detailed part that casts close to net shape and needs little machining, zinc usually wins on total cost — and the plating that zinc takes so well is part of that calculation, not an afterthought.

Corrosion sets the finish rule. Zinc is less noble than aluminum and sacrifices itself, so an unplated Zamak part outdoors shows white corrosion product within months. Every Zamak part we quote is therefore specified with a coating system: plating, powder coat or e-coat, with a thickness on the drawing. Choosing the alloy and choosing the finish are the same decision.

  • Small precision parts, hardware and lock components
  • Decorative and plated housings, bezels and covers
  • Thin-wall electronic and telecom fittings
  • Parts that need fine surface detail straight from the die
  • Insert-molded and over-molded components
02 / Capability

What the process holds, in numbers

Ranges we quote against for Zamak 3 and Zamak 5 on 160–800 T cold-chamber machines. The drawing still governs the part.

ParameterWorking rangeCondition that applies
Minimum wall0.5–0.8 mm0.5 mm on small parts with a short flow path; 0.8 mm on larger parts or long flow
As-cast tolerance±0.025 mmDimensions under 25 mm; ±0.05 mm above that
Machined tolerance±0.01 mmBores, faces and datums cut after casting
Draft0.5–1.5°0.5° minimum on deep walls and ribs
Casting shrinkage0.4–0.6%Tool geometry, bore spacing and pitch
Cycle time15–45 sSmall parts cool fast; die temperature sets the floor
Tool build15–25 daysFrom a released drawing; T1 samples 3–5 days after tryout
Capacity500,000+ parts / monthInstalled equipment across the partner plants
A dimension outside these ranges is not refused, it is reviewed: the answer names the change that would make it repeatable, and the cost or schedule it moves. The Zamak 5 mechanical properties page carries the strength and density values a drawing references.
03 / Design rules

The dimensions that decide a zinc tool

Zinc forgives thin walls and punishes a zero-draft plated face. These are the rules a DFM review checks first on a Zamak drawing.

FeatureWorking rangeWhy it matters
Wall thickness0.5–0.8 mm typical; 1.0–1.5 mm on load-bearing bossesThin walls fill easily in zinc; a wall that is too thin beside a boss still sucks metal and leaves a sink mark on the opposite face
Ribs0.4–0.6 mm at the root, tapering to about 0.3 mmRib roots stay under the wall thickness so the outer face does not sink; zinc fills ribs that aluminum would miss
Draft0.5° on walls, 1–1.5° on deep ribs and pocketsA plated part grows by the coating thickness; a 0° wall scuffs on ejection and scuffing shows through a cosmetic plate
FilletsR0.3–R0.8 mm at internal cornersA sharp corner is a stress riser and a fill problem at the same time; the fillet fixes both
Bosses and threadsBoss wall 0.8–1.2 mm; thread engagement 1.5× diameter in Zamak 5Zamak 5 holds a machine screw without an insert at moderate load; a thread in a 0.5 mm wall strips
Parting lineOff sealing faces and off the cosmetic faceFlash on a plated surface is removed by hand, and hand polishing shows as a witness line under chrome
Gate and overflowGate at the thickest section, overflow at last fillPorosity that reaches the surface blisters under plating; the gate and overflow layout is where it is prevented
InsertsKnurled or grooved, embed depth ≥ 1× insert diameterZinc grips an insert well; a shallow or smooth insert pulls out and is found only at assembly
These ranges describe common Zamak practice, not a substitute for the controlled drawing. Final wall, draft and insert position are confirmed in the DFM review against the part and the annual volume.
Six values a Zamak drawing carries: 0.5 to 0.8 mm wall, plus or minus 0.025 mm as-cast tolerance, Zamak 3 or 5, 0.5 degree minimum draft, copper-nickel-chrome finish and the release checks
Six values that decide whether a Zamak part casts, plates and passes inspection: wall, as-cast tolerance, grade, draft, coating system and the release checks each one is verified by.
04 / Plating

Plating is decided in the die, not on the line

A plating line can only coat what the die delivered. Porosity, cold shuts and a rough ejection mark become blisters or rejects two processes later.

FinishWhat it isWhat the drawing has to say
Copper–nickel–chromeDecorative plating, typically copper 10–15 µm, nickel 10–15 µm, chrome 0.2–0.5 µmThickness per metal, adhesion test, the cosmetic accept zone and the light it is inspected under
Powder coat60–90 µm polyester on a conversion-coated surfaceColor (RAL), gloss, thickness, masking and the cure schedule
E-coat15–25 µm epoxy, throws into recessesColor, thickness, and which threads and bores must stay clear
Zinc cannot be anodized: anodizing needs an aluminum substrate. A "clear anodized" note on a Zamak drawing comes back as a question at DFM, and the usual answers are bright plating, a clear lacquer over polished zinc, or a switch to aluminum.
05 / Grade choice

Zamak die casting grades: 3, 5, 2 and ZA-8

Copper is the variable. It raises strength and hardness, lowers ductility, and changes how evenly the part plates.

RequirementGradeWhy that grade
Dropped, struck or bent in serviceZamak 3About 10% elongation against 7% for Zamak 5: the difference between a dent and a crack
Threads, brackets, load-bearing fittingsZamak 5About 330 MPa tensile and 91 HB; roughly 20–30% stronger than Zamak 3
Highest strength in a small partZamak 2About 360 MPa, but 3% elongation and poorer dimensional stability make it a specialist choice
Bearing duty or warm serviceZA-88% aluminum raises high-temperature creep resistance; it needs tighter process control
Large flat decorative faceZamak 3The low copper level gives the most uniform plating and the fewest blisters
Zamak 3 and Zamak 5 run on the same 160–800 T machines with separate dies and process settings, so choosing one does not change the supplier. The Zamak 3 vs Zamak 5 comparison carries the full property table, the cost lines and the selection order.
06 / Inspection

What is checked before a plated part ships

Plating hides nothing for long: it blisters over porosity and shows every polishing mark. The checks below happen before the parts reach the plating line.

CharacteristicMethodFrequency
Melt chemistryOptical emission spectrometerEvery heat, against the alloy standard
DimensionsCMM at 0.001 mm on the drawing datumsFirst article, then a per-lot sample
Porosity under platingX-ray on critical and cosmetic zonesFirst article and cosmetic lots
Plating adhesionCross-hatch or thermal cyclePer plating lot
Coating thicknessXRF or coulometricPer plating lot, per layer
Corrosion resistanceNeutral salt spray, hours as agreedPeriodic, per finish system
A dimensional report leaves with every production lot. The acceptance criteria come from the drawing, not from a catalog.
Buyer questions

Zamak questions buyers ask first

Alloy, wall thickness and plating failures decide the price before the die is quoted.

Zamak is the standard alloy family used for zinc die casting: Zamak 3, 5 and 2, plus the higher-aluminum ZA-8. A drawing that says only “zinc die casting” leaves the grade to the caster, and the grade changes strength, ductility and plating behavior. Name the alloy and the standard.

Zamak 3 for decorative and plated parts that may be dropped or bent, because it plates more uniformly and has about 10% elongation. Zamak 5 where the part carries a thread, a bracket load or a wear face: about 330 MPa tensile and 91 HB. Parts that need both are reviewed at DFM rather than defaulted.

A small part with a short flow path casts at 0.5 mm; a larger part or a long flow needs 0.8 mm. Below 0.5 mm the fill becomes a capability question for that specific part, and it is answered with a trial rather than promised as a number.

No. Anodizing is an aluminum process; zinc has no anodic oxide of that kind. A Zamak part that needs a bright or colored finish is plated (copper–nickel–chrome), powder coated or e-coated, and the thickness goes on the drawing.

Subsurface porosity. Gas trapped in a pore expands through the plating cycle and lifts the coating. It is prevented in the die — gate position, overflow, die temperature and vacuum — and screened by X-ray on cosmetic parts before plating rather than reworked after it.

±0.025 mm on features under 25 mm and ±0.05 mm above that, with ±0.01 mm after machining. The class depends on the feature: a bore position across a long parting line is not the same call as a small pocket, and the drawing is where that is fixed.

Related pages

Continue through the project path.

The process, cost and quotation pages that belong to the same decision.

Thin-wall Zamak part with a plated finish?

Send the drawing with the grade, annual volume, plating specification and the cosmetic faces. DFM comes back with the wall, gate and porosity call before the die is quoted.