Material / Aluminum A380 (AlSi9Cu3(Fe))

A380 aluminum die casting: what the alloy does on the drawing

A380 is the default aluminum die casting alloy in North American drawings. It fills thin sections, holds pressure and machines predictably; the question is where it stops being the right call.

A380 Aluminum Die Casting material review A380 Aluminum Die Casting material review
7.5–9.5%
Silicon, the fluidity range
≈324 MPa
Typical as-cast tensile strength
2.71 g/cm³
Density, for part weight
650–700 °C
Melt temperature window
01 / Why this alloy

What A380 is actually chosen for

A380 is an Al-Si-Cu alloy, roughly AlSi9Cu3(Fe). The silicon sits around 8–9% and does one job well: it keeps the melt fluid long enough to fill thin walls before the gate freezes. The copper, 2–4%, buys strength and hardness after natural ageing, and takes ductility and corrosion resistance in exchange.

In a quotation review, A380 usually appears for three reasons: the part has walls between 1.0 and 2.0 mm, it has to hold air or oil, and it is machined on several faces. The alloy machines cleanly, holds a thread without tearing, and keeps dimensions after machining better than high-silicon alternatives. What that alloy choice does to the piece price is worked through line by line on the die casting cost page.

It is the wrong call when the part is seen anodized, when salt water is part of the service environment and no coating is specified, or when a drop or crash case has to be argued from elongation. Those are alloy decisions, and they belong on the drawing before the tool is quoted.

  • Housings and covers, roughly 0.3–4 kg per part
  • Pump and valve bodies that must hold pressure
  • Electronic and power enclosures with machined faces
  • Structural brackets that are not primary crash members
  • Parts where both casting and machining cost are audited
02 / Composition

Typical composition and what each element changes

Ranges follow the common A380 family specification. The mill certificate for the heat is the controlled document; a spectrometer check on the melt is what confirms it shot by shot.

ElementTypical range, wt%What it controls
Si7.5–9.5Fluidity and wear resistance. Above the range the eutectic coarsens and ductility falls
Cu2.0–4.0Strength and hardness after ageing. Raises hot shortness and lowers corrosion resistance
Mg≤ 0.30Strength through Mg2Si. Too much makes the melt pick up gas
Fe≤ 1.30Balances die sticking against brittle Al-Fe-Si plates. Too high and elongation collapses
Mn≤ 0.50Neutralises the iron plates. Too high and sludge settles in the furnace
Zn≤ 1.00Tramp element, tolerated. Raises hot shortness
Ni≤ 0.50Strength at temperature; usually present as tramp
Sn≤ 0.35Tramp element. Lowers strength and is best kept low
AlbalanceThe matrix
A certificate alone does not close the question: the casting's properties come from the melt plus the die. Chemistry, melt temperature and die temperature are recorded per shot family and reviewed when a lot fails a leak or X-ray check.
03 / Properties

Mechanical and physical properties, as cast

Values are typical for separately cast test bars. A production casting is not a test bar; porosity and wall thickness move these numbers.

PropertyTypical valueHow the drawing uses it
Ultimate tensile strength≈ 324 MPaSizing ribs, bosses and bolted joints
Yield strength, 0.2%≈ 159 MPaThread engagement and clamp load
Elongation≈ 3.5%Whether a drop or crash case can be argued at all
Hardness≈ 80 HBMachining feeds, wear at sliding faces
Density2.71 g/cm³Part weight from the 3D model
Thermal conductivity≈ 96 W/m·KMotor housings, heat spreaders
Melting range≈ 540–620 °CDie temperature, cycle time, soldering risk
For a pressure-tight part, the acceptance class in the drawing does more work than the alloy name: leak rate, X-ray zone and sectioning plan are what separate two suppliers quoting the same A380.
04 / Casting behavior

How A380 behaves inside the die

Fluidity and fill

Silicon-rich A380 fills 1.0 mm walls over flow lengths around 150–200 mm at a gate velocity of 30–60 m/s, provided the die runs at 180–250 °C. Below that die temperature the metal freezes in the runner and the last-filled corner shows cold shuts.

The practical consequence is that gate position, not alloy choice, decides whether a thin rib fills. A DFM review moves the gate before it suggests a different alloy.

Shrinkage and hot cracking

Linear shrinkage runs about 0.5–0.7%. Isolated thick sections freeze last and pull metal from the surrounding wall, which is where sink marks and shrinkage porosity appear. Ribs are kept at 0.6–0.8 of the adjacent wall and fillets at R1.5–R3 for that reason.

A380 is more tolerant of hot cracking than high-purity alloys because the copper-bearing eutectic fills the last interdendritic gaps, but it is not immune: sharp internal corners in a heavy section will crack on ejection if draft and fillets are ignored.

Porosity and pressure tightness

Two mechanisms matter. Gas porosity comes from turbulence and from hydrogen picked up by the melt; shrinkage porosity comes from the last region to freeze. A sealing face needs the gate to feed it, the overflow to take the cold metal, and often vacuum assistance to hold the leak rate.

Specify the leak rate and the test method, not the word airtight. Air decay at a defined pressure, water immersion with a defined observation time, or helium for the tightest parts — each changes the die design and the price.

05 / Machining and finishing

Machining, finishing and assembly notes

Machining

A380 cuts at 300–600 m/min with uncoated or PVD-coated carbide, high rake and air blast rather than flood coolant. Built-up edge is the usual defect, so sharp edges and a stable feed matter more than spindle speed.

Bores that carry bearings are finished in one setup from a single datum, because the as-cast position of a bore is not the position that matters. As-cast tolerance is around ±0.05 mm on small features, ±0.1 mm across a 200 mm housing; machined tolerance is ±0.01 mm.

Finishing

Powder coating, e-coat and chromate conversion all work on A380. Anodizing does not, in any cosmetic sense: copper and silicon produce a dark, patchy, uneven film. If the drawing says anodized, the alloy should be A360 or the finish should change.

Masking is a design decision. Threads, ground pads and EMC contact faces need masking, and masking cost scales with the number of masked features, not with their area.

Assembly and inserts

Threads are formed by machining or by cast-in inserts. In A380 a machined M6 thread needs at least 1.5× diameter engagement; below that, a helicoil or a self-clinching insert is cheaper than a pull-out claim.

Welding is not a production joining method for A380. Porosity and hot cracking make structural welds unreliable; adhesive bonding, inserts or a redesign hold the joint instead.

06 / Alternatives

Where A380 sits against the other alloys

The comparison that matters is rarely A380 against a better alloy; it is A380 against the alloy the customer's existing supplier already runs.

AlloyTensile, typicalElongationPick it when
ADC12≈ 310 MPa1–3%The drawing is Japanese or the supply chain is Asian; higher silicon gives slightly better fluidity and wear
A360≈ 317 MPa≈ 3.5%Corrosion resistance, ductility or anodizing is on the drawing
Zamak 3 (zinc)≈ 280 MPa10–15%Thin decorative walls and plating, at nearly three times the density
A380 and ADC12 are close enough that switching supplier rarely needs a drawing change; switching to A360 or to zinc is a design decision and should be reviewed with the tolerance and leak requirements in front of you.
07 / Inspection

What is checked on an A380 part

Inspection follows the risk in the drawing; the table is the default plan and is replaced by the customer's control plan where one exists.

CharacteristicMethodFrequency
ChemistrySpectrometer on the meltEvery heat
DimensionsCMM at 0.001 mm, or gaugesFirst article, then per-lot sample
Porosity in sealing zonesX-ray, plus sectioningFirst article and periodic
Pressure tightnessAir decay or water immersion100% where the drawing requires it
Cosmetic defectsApproved sample under agreed lightEvery lot
Threads and insertsGo/no-go gauge, pull test100% gauge, sample pull
Where a dimension cannot be measured after assembly, it is checked before assembly and the check is recorded. That ordering is written into the inspection plan, not left to the operator.
08 / Typical parts

Three parts where A380 earns its place

A gearbox or motor housing is the classic case: walls around 3–4 mm at the bearing bosses, porosity limits in the oil galleries, bores finished to ±0.01 mm and a leak test at the end. A380 fills the bosses, holds the pressure and machines the bores without tearing. Shapes from that family are worked through on the engine, water pump and battery housing page.

A pump or valve body adds internal pressure to the same problem. The gate has to feed the sealing face, and the inspection plan has to say which zones are X-rayed. A380's fluidity helps; the die design decides.

An electronic enclosure usually trades cosmetic quality against flatness: powder-coated outside, machined gasket land, threads for cable glands. A380 handles the machining and the coating, and the copper content stops mattering because nothing is anodized.

Buyer questions

A380 questions that change the quotation

Alloy grade, corrosion, machining and pressure tightness are the four answers that move a price.

No. They are close cousins from different standards. ADC12 allows more silicon (up to 12%) and often less copper; A380 allows 2–4% copper. In practice ADC12 fills slightly better and wears better; A380 is slightly more ductile and machines more easily. The drawing decides, and a substitution should be written down, not assumed.

Not in a cosmetic sense. Copper and silicon make the anodic film dark, patchy and uneven, so visible parts are powder coated, e-coated or chromate-treated instead. If the drawing requires anodizing, A360 is the alloy to quote, and the change should be agreed before tooling.

Not for structural joints. Porosity and hot cracking make weld strength unpredictable, and a certified weld procedure is unusual for high-pressure die castings. Inserts, adhesive bonding, or a redesign of the joint are the reliable routes; local cosmetic repair is a separate, documented decision.

About ±0.05 mm on small features measured from a stated datum, and around ±0.1 mm across a 200 mm housing, because draft, die wear and shrinkage all enter. Machined features are a different class: ±0.01 mm on a bearing bore is normal when the bore is finished in one setup.

By a leak rate at a stated pressure and method: air decay over a defined time, water immersion with an observation window, or helium for the tightest parts. The method changes the die, the cycle and the test cost, so it belongs on the drawing rather than in an email.

Related pages

Where this page connects.

Material, process, product and RFQ pages around the same decision.

Send the drawing. Get the engineering questions first.

Include the material, annual quantity, finishing requirement, target market and delivery date. The review can start from STEP, IGS, DWG, DXF, PDF or ZIP files.

Start an RFQ
Upload drawing