Projects / Thermal and enclosure parts

LED housings, camera casings and heat sinks: thermal parts and what decides them

An LED street light housing, a camera casing and a board-level heat sink look unrelated until the drawing is read: in all three the die-cast surface has to move heat, hold a gasket or both. Fin thickness, flatness of the contact pad and groove tolerance decide more than the alloy does.

Alloy
A380 / ADC12
Fin thickness
1.0–1.5 mm at root
Contact flatness
0.05 mm typical
Seal target
IP65–IP66 by design
Reference design

Reference design, not a delivered customer project.

This page describes a part family and the engineering decisions it forces. It is built from the geometry class and the process route, not from one customer order: no part number, customer name, delivery date, yield figure or measured result is shown.

Delivered project data is published only with the customer written authorization, and none of these images are customer photographs.

01 / Family

Three LED street light parts, one question: where does the heat go?

The family is defined by function, not by shape: each member conducts heat through a die-cast section and is judged on the surface that touches the hot component.

MemberAlloyTypical wallWhat decides acceptanceRelease test
LED street light housingADC122.5–3.5 mm, fins 1.0–1.5 mmFin fill; flatness of the LED contact pad; gasket groove sectionCMM flatness, air-decay seal test
Camera casingADC12 body + AL6063 extrusion2.5–3.0 mm bodyInterface between cast and extruded sections; anodizing uniformityCMM, color and finish sample
Medical circuit board heat sinkA3801.5–2.5 mm base, 1.0 mm finsFin straightness; base flatness; cleanliness before packingFlatness over the contact area, visual under agreed light
Contact flatness and fin geometry are quoted as typical values for this family. The drawing callout governs, and it is checked on the relaxed part.
02 / Context

Why thermal parts fail inspection.

A heat sink is not rejected because the fins look wrong; it is rejected because the base is not flat after the fins were cast, so the thermal interface material cannot fill the gap. The casting problem is the same on all three members: thin sections freeze first, the thick base freezes last, and the difference in shrink pulls the base out of flat.

  • Fins fill from the base, so gate so the base stays liquid longest
  • A 1.0 mm fin at the tip needs 1.5–2° draft or it drags on ejection
  • Flatness is specified on the contact area, not across the whole part
03 / Design

Four decisions for thermal castings.

These are the parameters that decide whether a thermal part performs and whether it can be coated.

Fin geometry

1.0–1.5 mm at the root, tapering to 0.8–1.0 mm at the tip, with 1.5–2° draft and a 2–3 mm gap between fins. Tighter than that and fill becomes the limit, not the die.

Base thickness

1.5–2.5 mm under the contact area is enough for a spreader; below 1.5 mm the base bows and the flatness callout becomes a machining operation instead of a casting one.

Contact surface

The pad that touches the LED or the board is usually machined or coined. Casting it flat to 0.05 mm is possible on a small pad and unrealistic on a 300 mm street light body.

Sealing and masking

A gasket groove and a coated exterior on the same part means masking. Groove depth is specified after coating, and the mask is part of the finishing specification, not an afterthought.

04 / Route

Casting route for a thermal part.

Sequence for this family, with the stage that decides thermal performance.

StageWhat happensControl point
DFM and thermal reviewFin geometry, base thickness, contact area and machining allowance agreedFin root and base thickness fixed before tooling
Die build and T1Gating to the base, venting at the fin tips, cooling layout for a thin-walled dieT1 fin fill and flatness on the relaxed part
MachiningContact pad faced or coined; mounting holes and groove cutFlatness on the pad, measured without clamping
Sealing or assemblyGasket fit, lens or board assembly where in scopeSeal test on the assembled housing where specified
FinishingPowder coat, anodizing or conversion coating with masking on the padPad flatness and continuity checked after finishing
Anodizing is a surface conversion, not a coating with thickness tolerance: it changes the dimension of the part slightly, which is why threaded and mating features are specified before anodizing.
05 / Failure modes

Where thermal castings go wrong.

Recurring causes on this family, with the change that removes them.

RiskMechanismCountermeasure
Short-filled fin tipsMetal freezes before the fin tip fillsWiden the gap to 2.5–3 mm, add overflow at the fin end, raise die temperature locally
Base bowed after ejectionThick base shrinks against thin finsEject on the base with a balanced pin layout, allow a stress-relief step before machining
Flatness lost after coatingCure temperature relaxes the castingMachine the pad after coating, or specify flatness after coating
Groove too shallowCoating thickness inside the grooveMask the groove or cut it after coating
Anodizing color variationCast and extruded sections take the dye differentlyAgree the sample on the actual mixed part, not on a coupon
06 / Inspection

What is checked on a thermal part.

Inspection concentrates on the surfaces that carry heat and the grooves that carry the seal.

CharacteristicMethodFrequency
Contact pad flatnessCMM or surface plate on the relaxed partEvery lot
Fin thickness and straightnessProfile gauge or sectionFirst article plus periodic audit
Base thicknessUltrasonic check or sectionFirst article plus periodic audit
Gasket groove sectionCMM or profile gaugeEvery lot
Seal integrityAir decay on the assembled housingWhere specified
Finish and colorApproved sample under agreed lightEvery lot
Appearance acceptance is settled on a physical sample under agreed light before the first production lot, because "matching the drawing" is not a usable criterion for a visible surface.
07 / Inputs

What a thermal casting quotation needs.

On this family the thermal requirement decides the geometry and the geometry decides the price. A quotation built without the heat load and the contact area is a price for a shape, and it usually changes after the first thermal test.

Send with the RFQ

  • Heat load, allowable case temperature and the contact area
  • Drawing with the flatness callout on the contact pad
  • Gasket specification and groove dimensions if already chosen
  • Finish: powder coat, anodizing, conversion coating, masking areas
  • Volume and whether assembly or sealing test is in scope
  • For mixed cast and extruded parts, the interface and the anodizing class
Buyer questions

Thermal and enclosure questions

What buyers ask about lighting, camera and heat sink castings.

On aluminum, 1.0–1.5 mm at the root tapering to 0.8–1.0 mm at the tip is the working range, with 1.5–2° draft and 2–3 mm between fins. Below 1.0 mm the fill becomes unreliable and the fin tends to short at the tip, which is worse for the thermal path than a slightly thicker fin.

On a small pad, yes, but it is not the economical route. On a street light body the pad is usually machined or coined after casting, because the base moves when the part is released from the die and again during coating. We specify flatness on the machined pad and measure it unclamped.

The cure cycle heats the part to 180–200 °C, which is enough to relax residual stress from the casting and move a thin base. The two ways out are to machine the pad after coating or to specify and check flatness after coating, and both have to be written into the drawing before the first lot.

Yes, and the camera casing in this family does exactly that: a die-cast body for the geometry that cannot be extruded, an aluminum extrusion for the constant section, and CNC machining and anodizing across both. The risk is color match after anodizing, because cast and extruded alloys dye differently, so the sample is approved on the assembled part.

The LED module footprint and its mounting pattern, the gasket concept, the IP target, the finish and the annual volume. Without the module footprint the contact pad is a guess, and the thermal performance of the whole fixture depends on that pad.

Send the module footprint and the housing drawing.

We answer within 30 minutes during Shenzhen business hours with a price direction or the questions we still need answered.

Start an RFQ
Upload drawing